P.539
| FIBER PROTECTOR TEST RESULTS |
| 1.TENSILE STRENGTH TEST | 2.COMPRESSION BREAKING LOAD TEST | 3.BEND-BREAKING LOAD TEST | 4.TEST CERTIFICATE |
1.TENSILE STRENGTH TEST: FIBER PROTECTOR
| METHOD OF TEST | PURPOSE OF THE TEST |
| COMPRESS 200mm FIBER PROTECTOR 10mm/MINUTE UNTIL IT BREAKS. THE RESULT ON THE TABLE IS WEIGHT OF BREAKING POINT. |
TO GET DATA OF TENSILE STRENGTH ON SECTION (b). |
![]() |
![]() |
| RESULTS | |||
| TYPE | Range/kg | WEIGHT OF BREAKING POINT kg | MEMO |
| KS-1.5N | 500 | 23.0 | * |
| KS-1.8N | 500 | 20 | * |
| KS-2.2N | 500 | 23 | * |
| KS-3N | 500 | 39.2 | * |
| KS-4N | 500 | 69.1 | * |
| KS-5N | 500 | 60 | * |
| KS-6N | 500 | 73.2 | * |
| KS-7N | 500 | 68.2 | * |
| KS-8N | 500 | 94 | * |
| KS-9N | 500 | 80.1 | * |
| KS-13N | 500 | 87.3 | * |
| KS-15N | 500 | 70.4 | * |
| KSP-4N | 500 | 74.5 | CASING +PVC |
| SA-4N | 500 | 106 | * |
| SA-8N | 500 | 130 | * |
| SX-5N | 500 | 130 | * |
| SX-8N | 500 | 224 | * |
| IS-9N | 500 | 220 | * |
| SASP-8.5N-0,9 | 500 | 124 | * |
| SAP-8N | 500 | 140 | SEMI-INTER+PVC |
| SABP-8N | 500 | 230 | SEMI-INTER+IRON BRAIDED |
|
These tests were performed by IS-10T and RS-2 made by Shimazu Co., Ltd
at Chibaken Mechanical-Metal Examination Institute and Tokyo-Metropolitan-Mechanical-Technology
Center on 08/28/1989. |
|||